Welding Corten Steel: Thin Gauge vs Thick Plate Practice

Dec 25, 2025 Leave a message

How Gauge Changes the Welding Task

Weathering steel is welded with the same equipment as ordinary structural carbon steel, but the working window narrows, and it narrows in opposite directions at the two ends of the thickness range. Thin sheet of 3 mm and under is dominated by the risk of burn-through, distortion and loss of the weathering chemistry in an oversized heat-affected zone. Thick plate of 5 mm and over is dominated by the need for full penetration, adequate heat input and interpass control to avoid cracking and loss of toughness.

The grades involved, including SPA-H to JIS G3125, Q355NH to GB/T 4171, A588/A588M, A606 Type 4 and S355J2W to EN 10025-5, all rely on copper, chromium and nickel additions for their corrosion behaviour, and the weld metal must contain a comparable alloy content or the joint will corrode preferentially before the parent plate.

Process Selection and Heat Input

Parameter Thin gauge (3 mm and under) Thick plate (5 mm and over)
Preferred processes GTAW (TIG) or MAG with short-circuit transfer SMAW, MAG with spray transfer, SAW for long runs
Heat input 0.5-1.2 kJ/mm 1.5-3.0 kJ/mm
Filler diameter 1.6-2.4 mm (MAG), 2.0-2.5 mm (GTAW) 3.2-4.0 mm (SMAW), 2.4-4.0 mm (SAW wire)
Current range 60-120 A 180-300 A
Passes Single pass where possible Multi-pass with full penetration
Interpass temperature Keep low, monitor distortion 150 deg C maximum

Oxyacetylene welding is not recommended on thin weathering sheet because the heat input is excessive and the flame chemistry does not suit the alloy. On thick plate, submerged arc welding is efficient for straight, long seams such as stiffener-to-web connections, and it gives consistent penetration when the flux and wire combination is matched to the parent analysis. Interpass temperature control is critical on thick sections: allowing the joint to run hot coarsens the grain structure in the heat-affected zone and reduces both toughness and corrosion resistance.

Joint Design and Preparation

Thin sheet is welded with lap or butt joints, square edged or with a small 30 degree bevel, so that the weld volume stays small and the plate does not distort. Fit-up must be tight, with a gap of no more than about 0.5 mm, because any wider opening either burns through or requires extra filler that increases shrinkage. Tack welds should be short and spaced, and backing strips, where used, must be removed or fully sealed afterwards, since a trapped crevice is a permanent corrosion site.

Thick plate uses single-V or double-V preparations with a 60-70 degree included angle, which gives the welder access to the root while keeping the deposited volume manageable. Roots should be cleaned of rust, oil and scale before welding, and a root gap of about 2-4 mm is used for multi-pass work. Back gouging and sealing runs are used where full penetration is required, and the completed groove should be free of slag inclusions and lack of fusion, which are the two defects that most often become corrosion initiation points.

Filler Metals and Corrosion Continuity

Filler selection is what separates a weathering steel weld from an ordinary carbon steel weld. The consumable must deposit weld metal with a copper, chromium and nickel content comparable to the parent plate so that the joint develops a similar oxide layer. A gas-shielded wire of ER80S-G chemistry with nickel, copper and chromium additions is typical for MAG and GTAW work, and a low-hydrogen electrode of similar analysis is used for manual metal arc welding. Where the parent plate is an A-type phosphorus grade, welding is generally avoided in favour of mechanical connections, because the high phosphorus content raises the risk of hot cracking; this is one reason B-type chemistry, with lower phosphorus and added nickel, is preferred for welded assemblies.

Two further points follow from the chemistry. First, the weld cap should be cleaned and brushed so that its surface condition matches the parent plate and drains freely. Second, temporary attachments and lifting lugs must be welded with the same consumables and removed by cutting well clear of the surface, never by hammering, which damages the plate and leaves a crevice.

Inspection and Post-Weld Treatment

Visual inspection for undercut, spatter, crater cracks and cap profile, then dimensional checks on set-up and distortion.

Dye penetrant or magnetic particle examination on fillet and partial penetration joints, with ultrasonic or radiographic testing where the procedure requires full penetration verification.

Hardness or microstructural checks on thick-section heat-affected zones where toughness is a design requirement.

Grinding or brushing of the weld and its surroundings so no crevice, spatter or embedded iron remains.

Confirmation that no carbon steel fastener, tool mark or temporary weld has been left on the finished face.

Documentation for welded weathering steelwork should include the material certificates to EN 10204 type 3.1, a qualified welding procedure specification with its supporting procedure qualification record, filler metal certificates, and the inspection records. Once the assembly is complete, the joint should be left uncoated so it oxidises with the parent plate; a paint stripe over a weld on an unpainted weathering structure will simply become a visible patch that fails before the surrounding oxide stabilises.

Frequently Asked Questions

Q: Is Corten steel harder to weld than ordinary carbon steel?

A: The technique is similar, but the process window is narrower and the filler metal must match the weathering chemistry. Thin sheet demands strict heat control to avoid burn-through, and thick plate demands interpass temperature limits to protect toughness.

Q: What heat input is suitable for thin Corten sheet?

A: Roughly 0.5-1.2 kJ/mm using GTAW or short-circuit MAG with small-diameter filler and 60-120 A. This keeps the heat-affected zone narrow and prevents warping and melt-through.

Q: Which filler metal should be used?

A: A consumable depositing copper, chromium and nickel in comparable amounts to the parent plate, such as an ER80S-G type wire for gas-shielded processes or a low-hydrogen electrode of similar analysis for manual metal arc welding.

Q: Can submerged arc welding be used on weathering plate?

A: Yes, on thick plate and long straight seams, with a wire and flux combination matched to the parent analysis. It suits stiffener-to-plate and web-to-flange joints where consistent penetration and productivity matter.

Q: Why is an A-type phosphorus weathering grade harder to weld?

A: The higher phosphorus content increases the risk of hot cracking in the weld and heat-affected zone, so welded assemblies normally use the low-phosphorus B-type chemistry instead, and A-type material is reserved for mechanical connections and flat panels.

Q: Should welded joints be painted or sealed afterwards?

A: No, on an unpainted weathering structure. The weld should be cleaned, dressed and left bare so it develops an oxide layer at the same rate as the surrounding plate; a local coating would create an appearance mismatch and an eventual failure point.