ASTM A847 Electric Resistance Welded Pipe

Nov 24, 2026 Leave a message

What Is ASTM A847 Electric Resistance Welded Pipe?

ASTM A847 is a standard specification covering cold-formed welded and seamless high-strength, low-alloy structural tubing with improved atmospheric corrosion resistance.

 

It applies to round, square, rectangular, and specially shaped structural tubing used in welded, riveted, or bolted construction of bridges, buildings, and other structural applications. ASTM A847/A847M-21 is an applicable published edition of this specification.

 

ASTM A847 Electric Resistance Welded Pipe is manufactured by forming steel strip or plate into a tubular shape and joining the longitudinal edges through electric resistance welding (ERW). 

 

As a manufacturer and supplier of weathering steel products, we provide ASTM A847 ERW steel pipe and tubing for structural applications requiring a minimum yield strength of 50 ksi (345 MPa) and a minimum tensile strength of 70 ksi (485 MPa).

 

The specified minimum elongation is 19% for wall thicknesses of 3.0 mm and above. For thinner walls, elongation requirements are subject to agreement with the manufacturer.

 

ASTM A847 weathering steel contains copper as a specified alloying element, with a minimum heat-analysis content of 0.20%. Nickel, chromium, and silicon contents are also reported in the material analysis.

 

The standard requires an atmospheric corrosion resistance index of at least 6.0, calculated in accordance with ASTM G101. These requirements make A847 suitable for structural projects exposed to atmospheric conditions where reduced maintenance associated with weathering steel is required.

 

Our ASTM A847 electric welded tubing can be supplied in round, square, and rectangular configurations according to project drawings and purchasing specifications.

 

Available dimensions, wall thicknesses, lengths, weld seam requirements, and end preparations are confirmed before production. Each order can be accompanied by a Material Test Certificate (MTC) containing chemical composition, mechanical test results, and product identification information.

ASTM A847 electric resistance welded steel pipe
ASTM A847 electric welded tubing

If you are sourcing ASTM A847 electric resistance welded steel pipe for bridge structures, building frameworks, outdoor structural supports, or industrial fabrication, please send us your required outside diameter or section dimensions, wall thickness, quantity, and length. Our sales and technical teams will review the requirements and prepare a project-specific quotation.

 

ASTM A847 Electric Resistance Welded Pipe Specification

ASTM A847 covers welded and seamless high-strength, low-alloy structural tubing. The following table summarizes the main specification requirements and typical procurement information for ASTM A847 ERW steel pipe. 

Item

Specification / Details

Standard

ASTM A847 / ASTM A847M

Manufacturing Process

Cold-Formed Electric Resistance Welding (ERW)

Minimum Yield Strength

50,000 psi / 345 MPa

Minimum Tensile Strength

70,000 psi / 485 MPa

Minimum Elongation

19% (wall thickness ≥ 3.0 mm)

Corrosion Resistance Index

≥ 6.0 (ASTM G101 calculation)

 

ASTM A847 ERW Steel Pipe Chemical Composition

ASTM A847 specifies chemical requirements for carbon, manganese, phosphorus, sulphur, and copper. Nickel, silicon, and chromium contents must also be reported, although the standard does not prescribe minimum values for these three elements. The copper minimum does not apply when both chromium and silicon are at least 0.50%.

 

The following values are based on ASTM A847/A847M-21, Table 2. All values are percentages by mass.

Element

Heat Analysis (%)

Product Analysis (%)

Carbon (C)

0.20 max

0.24 max

Manganese (Mn)

1.35 max

1.40 max

Phosphorus (P)

0.04 max

0.04 max

Sulphur (S)

0.035 max

0.045 max

Copper (Cu)

0.20 min

0.18 min

Nickel (Ni)

Reported

Reported

Silicon (Si)

Reported

Reported

Chromium (Cr)

Reported

Reported

 

Mechanical Properties of ASTM A847 Weathering Steel Tube

ASTM A847 requires round and shaped structural tubing to meet specified minimum tensile properties. These requirements apply to both welded and seamless products covered by the standard.

Mechanical Property

Requirement

Metric Unit

Yield Strength

50,000 psi min

345 MPa min

Tensile Strength

70,000 psi min

485 MPa min

Elongation in 2 in. (50 mm)

19% min

19% min

Elongation note: The 19% minimum elongation requirement applies to specified wall thicknesses of 0.120 in. (3.0 mm) and above. 

 

These mechanical requirements make ASTM A847 ERW steel pipe suitable for structural members that require a minimum yield strength of 345 MPa and tensile strength of 485 MPa.

 

ASTM A847 ERW Pipe Dimensional Tolerances

Dimensional accuracy is an important consideration when purchasing electric resistance welded pipe for structural fabrication. ASTM A847 specifies permissible variations for outside diameter, section dimensions, wall thickness, straightness, length, squareness, corner radius, and twist.

1. Round ASTM A847 ERW Steel Pipe

Nominal Outside Diameter

Permissible OD Variation

≤ 48.3 mm (1.900 in.)

±0.5%

≥ 50.8 mm (2.000 in.)

±0.75%

The outside diameter is measured at least 50.8 mm (2 in.) from either end of the tubing.

 

2. Square and Rectangular ASTM A847 Tubing

Largest Outside Dimension Across Flats

Permissible Variation

≤ 63.5 mm (2.5 in.)

±0.5 mm

63.5–88.9 mm (2.5–3.5 in.)

±0.6 mm

88.9–139.7 mm (3.5–5.5 in.)

±0.7 mm

> 139.7 mm (5.5 in.)

±1%

These tolerances include allowances for convexity and concavity. For rectangular sections, the tolerance calculated for the larger flat dimension also applies to the smaller dimension, subject to the standard's provisions for increased tolerance in certain aspect ratios.

 

3. Wall Thickness Tolerance

Parameter

Permissible Variation

Minimum Wall Thickness

90% of specified wall thickness

Maximum Wall Thickness

110% of specified wall thickness

The maximum wall thickness requirement excludes the weld seam of welded tubing. For square and rectangular tubing, wall thickness is measured at the center of the flat.

 

4. Other Dimensional Requirements

Parameter

ASTM A847 Requirement

Straightness

1/8 in. per 5 ft (10.4 mm per 1.5 m)

Squareness of Adjacent Sides

Maximum deviation of 2° from 90°

Outside Corner Radius

Maximum 3 × specified wall thickness

Length

Random, multiple, or specified mill lengths

Twist

According to the applicable ASTM A847 tolerance table

Our team can review these details before production and confirm the applicable manufacturing tolerances.

 

ASTM A847 Electric Resistance Welded Tubing Manufacturing Process

ASTM A847 electric resistance welded tubing is produced through a continuous cold-forming and welding process. The main manufacturing stages are as follows:

1. Raw Material Selection and Inspection

Steel coils or strips are selected according to ASTM A847 chemical and mechanical requirements. Material identification, heat numbers, thickness, width, and surface condition are checked before production.

 

2. Strip Slitting

The steel coil is slit into strips of the required width according to the finished pipe dimensions and forming specifications.

 

3. Cold Forming

The steel strip passes through a series of forming rolls to gradually create a round tubular section. For square and rectangular tubing, additional sizing and forming operations are performed to achieve the specified cross-sectional dimensions.

 

4. Electric Resistance Welding

The longitudinal edges of the formed strip are heated by electrical resistance and joined under pressure to create a continuous weld seam. This process produces ERW steel pipe without the use of filler metal in conventional high-frequency ERW production.

 

5. Sizing and Straightening

After welding, the tube passes through sizing rolls to achieve the specified outside diameter or section dimensions. Straightening operations are performed to control the finished tube's alignment.

 

6. Cutting and End Preparation

The continuous tube is cut into the required random or specified lengths. Plain ends, beveled ends, or other agreed end preparations can be provided according to the purchase order.

 

7. Inspection and Testing

Finished ASTM A847 electric welded tubing is inspected for dimensional accuracy, surface condition, mechanical properties, and compliance with the applicable standard. Additional testing can be arranged according to project requirements.

ASTM A847 electric welded tube
A847 Electric Resistance Welded Steel Pipe
A847 Welded Steel Pipe

Applications of ASTM A847 Electric Resistance Welded Steel Pipe

ASTM A847 electric resistance welded steel pipe is used in structural projects where high strength and improved atmospheric corrosion resistance are required. Its round, square, and rectangular profiles provide options for different structural configurations.

 

1. Bridge Structures

ASTM A847 ERW steel pipe and structural tubing can be used in bridge components, supporting structures, and fabricated members where the design specifies high-strength weathering steel. The material's minimum yield strength of 345 MPa supports structural load-bearing requirements.

 

2. Building Frameworks

Square and rectangular ASTM A847 tubing can be used in building frameworks, structural columns, support members, and architectural steel structures. Section dimensions can be selected according to engineering drawings and load calculations.

 

3. Outdoor Structural Supports

ASTM A847 weathering steel tubing is suitable for outdoor structural components exposed to atmospheric conditions, including support frames, equipment structures, and other exposed steel assemblies.

 

4. Industrial Structural Fabrication

ERW steel pipe can be fabricated into industrial support frames, equipment bases, platforms, and other structural components. Its cold-formed sections are suitable for cutting, drilling, welding, and assembly according to the fabrication procedure.

 

5. Architectural and Landscape Structures

ASTM A847 square steel tubing and rectangular steel tubing can be incorporated into outdoor architectural frameworks, landscape structures, and exposed steel installations where weathering steel is specified.

 

Testing and Inspection of ASTM A847 ERW Steel Pipe

Quality control is essential for ASTM A847 electric resistance welded steel tubing. Inspection procedures should cover chemical composition, mechanical properties, dimensions, surface condition, and weld-related requirements.

Inspection Item

Testing / Inspection Method

Chemical Composition

Heat Analysis / Product Analysis

Tensile Properties

Tensile Test

Round Tube Flattening

Flattening Test

Outside Diameter

Dimensional Measurement

Wall Thickness

Thickness Measurement

Section Dimensions

Dimensional Measurement

Straightness

Straightness Measurement

Surface Condition

Visual Inspection

Weld Seam

Visual / Agreed NDT

Material Traceability

Heat Number and MTC Review

 

 

Lead Times and Packaging

We support procurement requirements for ASTM A847 electric resistance welded pipe, including project-based orders and customized structural tubing.

 

Production lead time depends on section dimensions, wall thickness, material availability, order quantity, and inspection requirements. The delivery schedule is confirmed after technical specifications and order details are finalized.

 

Before shipment, pipes and tubes are inspected, bundled, and packed according to their dimensions and transportation requirements.

 

Protective materials and suitable packaging are used to reduce the risk of surface damage, deformation, and contamination during handling and international transportation.

ASTM A847 electric resistance welded pipe
A847 electric resistance welded pipe
ASTM A847 welded pipe

Request A Quote For ASTM A847 Electric Resistance Welded Pipe

 

Are you looking for ASTM A847 ERW steel pipe, electric resistance welded tubing, or cold-formed welded pipe for a bridge, building, or outdoor structural project? Please send us the following information:

Material Standard: ASTM A847 / ASTM A847M

Product Shape: Round / Square / Rectangular / Special Shape

Outside Diameter or Section Size: OD / Width × Height

Wall Thickness: mm or inch

Required Length: Fixed Length / Random Length

Quantity: Tons or Pieces

Inspection Requirements: Standard Inspection / Third-Party Inspection

Documentation: MTC / Chemical Analysis / Mechanical Test Report

 

Our team will evaluate your requirements, confirm production feasibility, and provide a quotation covering product specifications, inspection arrangements, packaging, and delivery terms.

 

Get Your ASTM A847 ERW Steel Pipe Quotation Today!