Differences between S235J0 steel and S235J0W weathering structural steel sheet

Oct 28, 2025 Leave a message

The difference between S235J0 and S235J0W is that S235J0 is a carbon structural steel and the standard is EN 10025-2. S235J0W is weathering structural steel, the standard is EN 10025-5.

 

S235J0W

 

The difference in chemical composition

 

 

EN 10025-2 S235J0 steel plate chemical composition

Grade Chemical Composition
S235J0 The Element Max (%)
C Si Mn P S N Cu
≤16 >16≤40 >40
0.19 0.19 0.19 - 1.50 0.040 0.040 0.014 0.60

 

EN 10025-5 S235J0W steel chemical composition (%)

Grade Number C max. Si max. Mn P S max. N max. Cr Cu
S235J0W 1.8958 0.13 0.40 0.20 - 0.60 max. 0.035 0.035 0.009 0.40 - 0.80 0.25-0.55

 

The difference in mechanical properties

 

 

EN 10025-2 S235J0 steel plate mechanical properties

Grade Mechanical Property
S235J0 Yield Strength
mm
Min Mpa
Tensile Strength
mm
Min Mpa
≤16 >16
≤
40
>40
≤
63
>63
≤
80
>80
≤
100
>100
≤
150
>150
≤
200
>200
≤
250
>250
≤
400
<3 ≥
3
≤
100
>100
≤
150
>150
≤
250
>250
≤
400
235 225 215 215 215 195 185 175 - 360-510 360-510 350-500 340-490 -

 

EN 10025-5 S235J0W steel plate mechanical properties

EN 10025-5 Min. Yield Strength Reh MPa Tensile Strength Rm MPa
Nominal Thickness (mm) Nominal Thickness (mm)
≤16 >16 ≤40 >40 ≤63 >63 ≤80 >80 ≤100 >100 ≤150 <3 >3 ≤100 >100 ≤150
S235J0W 235 225 215 215 215 195 360-510 360-510 350-500

 

The difference in application

 

S235J0 European standard carbon structural steel, 0°C impact, S235J0 is used to manufacture welding, bolting and riveting structures. S235J0W is a weather-resistant structural steel improved on the basis of S235J0.

 

S235J0W is used for welding, bolting and riveting parts. This steel grade enhances the ability to resist atmoSPHEric corrosion at ambient temperature.

 

It is added in order to achieve corrosion resistance. Certain specific alloying elements, such as P, Cu, Cr, Ni, Mo, etc., form a protective oxide layer on the metal surface under various climatic conditions.

 

Contact now to get S235J0W Quote

 