SPA-H Steel Plate Delivery State: Annealed or As-Rolled?

Dec 25, 2025 Leave a message

SPA-H and the JIS G 3125 Delivery Framework

SPA-H is the hot-rolled atmospheric corrosion resisting steel grade defined in JIS G 3125, the Japanese standard for superior atmospheric corrosion resisting rolled steels. It is the grade most often ordered for shipping containers, sign gantries, guardrails, rail wagon panels, bridge parapets and exposed architectural plate, because it is designed to be left unpainted in open-air service where wet and dry cycles allow a protective oxide layer to densify. JIS G 3125 controls the chemical window and the mechanical floor values that a mill must certify: copper in the 0.25 to 0.55 percent range, chromium between 0.30 and 1.25 percent, a maximum carbon content of 0.12 percent, and phosphorus deliberately held in the 0.070 to 0.150 percent band so that the patina forms quickly and stays adherent.

Mechanical requirements are written as a minimum tensile strength of 490 MPa and a minimum yield strength of 355 MPa, with minimum elongation stepped by product thickness. Because the standard describes the steel rather than a heat treatment, the delivery condition is fixed by the product form and by what the purchase order states, not by one mandatory process route. Suppliers therefore quote a delivery state explicitly, and that state appears on the mill certificate together with heat number, dimensions and mechanical test results.

Standard Delivery States for Hot-Rolled SPA-H Plate and Coil

For hot-rolled SPA-H the default delivery states are as-rolled (AR) and thermo-mechanical controlled processing (TMCP). In the as-rolled condition the slab is rolled above the recrystallisation temperature and then allowed to cool naturally, producing a stable ferrite-pearlite microstructure with predictable strength and ductility for outdoor load-bearing work such as large sign structures, guardrail beams and container components. In the TMCP condition, controlled rolling is combined with accelerated cooling, which refines the ferrite grain size and improves the strength and toughness balance without adding a separate heat treatment step.

Rolling and finishing options offered against a JIS G 3125 order typically include:

Hot-rolled black, unpickled, mill scale intact, for direct fabrication.

Pickled and oiled, for painting lines, laser cutting and press work where clean surfaces are needed.

TMCP, for heavier gauges and for structures that need tighter toughness control.

Cold-rolled, for thin strip and sheet below the normal hot-rolled gauge range.

Annealed, quoted only as a priced additional operation.

Thickness, width, flatness and camber are checked against the dimensional tolerances referenced by the order, and ultrasonic or visual inspection can be added for plate intended for pressure-adjacent or fatigue-loaded details.

Cold-Rolled SPA-H Strip: Delivery Without Annealing

Thin SPA-H is normally supplied cold-rolled (CR) and not annealed. Cold reduction is carried out at ambient temperature using hot-rolled SPA-H as the base material, which plastically deforms the lattice, raises hardness through work hardening and slightly reduces ductility while improving surface finish, flatness and dimensional accuracy. The cold-rolled condition suits decorative panels, small precision components and thin cladding elements in the 0.3 mm to 3 mm gauge band, where appearance and forming accuracy matter more than the highest possible elongation.

Work hardening has two practical consequences for the buyer. First, tight bend radii that are harmless on hot-rolled plate can cause edge cracking on cold-rolled strip, so minimum bend radius must be agreed before shearing. Second, hardness variation across a coil is normal and shows up in laser cutting kerf width and in roll forming. Neither issue requires annealing, but both must be reflected in the tooling and in the drawing tolerances.

Annealing as a Purchased Additional Treatment

Annealing becomes relevant only when the buyer writes a specific performance or processing requirement into the order. Two routes are common:

Full annealing. The material is heated into the 850 to 900 degree C range, held long enough for recrystallisation, then cooled slowly. This removes cold-rolling work hardening, softens the steel and restores ductility for severe bending, deep drawing, stamping or welding sequences.

Process annealing. A lower-temperature treatment in the 550 to 650 degree C range applied to cold-rolled strip to relieve internal stress without collapsing the strength level, used where hardness and formability must be balanced.

An annealed delivery is never the default and it changes commercial terms as well as metallurgy. It adds a heat treatment operation to the route, which raises the unit price and extends the lead time, and it means the mechanical certificate must be tied to the post-anneal test results rather than to the rolling results. For that reason the treatment has to be stated as an explicit line item in the purchase contract, together with the target properties, otherwise the mill is entitled to ship the standard as-rolled or cold-rolled condition.

Delivery Documentation, Tolerances and Quality Control

A well-written SPA-H order removes the ambiguity that causes most delivery disputes. The specification should state grade, standard, product form, delivery state, dimensions with tolerances, edge condition, surface requirement and the tests to be witnessed. Each shipment should travel with a certificate of inspection showing heat number, chemical analysis, tensile and yield results, elongation and, where relevant, impact values, plus a statement of the delivery state actually applied.

Incoming goods checks for fabricators are straightforward: verify the heat number against the certificate, confirm thickness at several points across the plate, check flatness and camber against the agreed tolerance, and record surface condition before any cutting. Material that will be welded into critical details should also be checked for the absence of laminations at the edges, since edge laminations are a fabrication risk rather than a corrosion issue. Where plate is ordered for a coating line, mill scale adhesion should be reviewed before blasting, because the chemistry and cooling path of SPA-H both influence scale behaviour.

Selecting the delivery state is therefore a functional decision. Outdoor load-bearing plate ordered as as-rolled or TMCP performs exactly as intended without annealing. Cold-rolled strip that will be bent aggressively, or components that must be stress relieved after forming, are the cases that justify a written anneal requirement.

Frequently Asked Questions

Q: Is annealing the standard delivery state for SPA-H steel plate?

A: No. According to JIS G 3125 the normal delivery conditions are as-rolled or TMCP for hot-rolled plate and cold-rolled for thin strip. Annealing is an optional additional treatment quoted only when it is specified in the order.

Q: What mechanical properties must a JIS G 3125 SPA-H certificate show?

A: A minimum yield strength of 355 MPa and a minimum tensile strength of 490 MPa, with minimum elongation that varies with product thickness, plus chemical analysis confirming the copper, chromium, phosphorus and carbon levels required by the grade.

Q: Does annealing change the corrosion performance of SPA-H?

A: It changes the surface condition rather than the alloy content. An annealed surface is cleaner and more uniform, which allows a more even patina to develop, but the corrosion resistance still depends on the copper, chromium and phosphorus additions being present as specified.

Q: Why does a cold-rolled SPA-H strip crack when it is bent?

A: Cold reduction work hardens the steel, so tight bend radii that are acceptable on hot-rolled plate can cause edge cracking. The remedy is a larger bend radius, an agreement on mechanical properties at the drawing stage, or a request for process annealing.

Q: How long does an annealed order take compared with a standard rolling?

A: An annealed delivery adds one heat treatment operation and the associated testing to the production route, so the lead time and the unit price both increase. The exact extension depends on the mill schedule and should be confirmed in the contract.

Q: Can plate be supplied half in the as-rolled condition and half annealed from the same heat?