Degrease the surface with anhydrous ethanol or neutral degreaser; wipe loose rust/scales with a soft nylon brush, then air-dry.
Prepare pickling solution: 5–10% dilute hydrochloric acid/8–12% phosphoric acid + 0.2–0.5% corrosion inhibitor (e.g., urotropine), keep at 20–30°C.
Wear acid-resistant gloves, goggles, and operate in a well-ventilated area.

Immersion method: Submerge the plate fully for 10–20 minutes until the surface turns uniform silvery-gray (stop if oxide scales disappear; avoid over-pickling >30 mins).
Spray method (for large plates): Spray acid solution evenly for 8–15 minutes, keeping the surface moist.

Rinse the plate thoroughly with clean water, then neutralize in 2–3% sodium hydroxide solution for 2–3 minutes.
Rinse again and dry completely within 10 minutes using a blower/hot air dryer (prevent flash rust).

For natural patina use: Apply rust stabilizer/patina accelerator within 1 hour; cure 24–48 hours at room temperature.
For coating use: Apply compatible primer (e.g., epoxy zinc-rich primer) within 4–6 hours.

Key Notes
Do not stack plates before post-treatment; dispose of waste acid after neutralizing to pH 6–8.