1. Toughness: Significant Improvement (30–50% Increase)

 

Core change: Room-temperature Charpy V-notch impact toughness rises from a baseline 40–50 J to 60–75 J for all initial states, the most pronounced effect of normalizing.

Mechanism: Fine equiaxed ferrite-pearlite grains (20–35 μm, 50–60% refined vs. hot-rolled coarse grains) absorb impact energy more effectively than coarse/elongated grains or work-hardened distorted microstructures.

Practical value: Eliminates brittle fracture risk, critical for structural SPA-H components (bridge railings, support columns) exposed to dynamic loads, low temperatures, or outdoor impact (wind-blown debris, mechanical contact).

info-376-294

2. Ductility/Elongation: Noticeable Increase (Restores Formability)

 

Hot-rolled SPA-H: Elongation at break (≥20% baseline) rises by 8–12% to ≥22–24%, enhancing formability for bending/curving without cracking.

Cold-rolled SPA-H: Work hardening-induced low elongation (≤15% baseline) is restored to 18–20% (a 20–33% increase), reversing excessive ductility loss while retaining partial cold-rolled strength.

Welded SPA-H: Elongation in the heat-affected zone (HAZ) is homogenized to match the base metal (≥20%), eliminating ductility disparities that cause weld joint cracking.

Mechanism: Recrystallization of distorted grains and annihilation of tangled dislocations (from cold rolling/welding) restore the steel's ability to deform plastically.

info-639-506

3. Strength: Moderate, Controlled Reduction (Still Meets JIS Minimum)

 
Normalizing slightly reduces yield and tensile strength by relieving stress-induced hardening and refining grains (fine grains boost toughness but lower strength marginally), yet all values remain above the JIS G 3125 minimum 345 MPa yield strength (345 MPa min, 480 MPa min tensile).
 

Hot-rolled SPA-H: Yield strength (360–420 MPa baseline) drops 5–10% to 340–380 MPa; tensile strength (480–620 MPa baseline) drops 3–5% to 460–590 MPa.

Cold-rolled SPA-H: Work-hardened high strength (415–450 MPa yield, 550–600 MPa tensile baseline) drops 12–20% to 360–380 MPa yield / 480–520 MPa tensile-partial reversal of work hardening for a strength-ductility balance.

Welded SPA-H: Strength in the coarse-grain HAZ (elevated from rapid weld cooling) is reduced to match the base metal, eliminating strength imbalances in weld joints.

info-213-175

4. Hardness: Mild Reduction (Correlates with Strength Loss)

 

Hot-rolled SPA-H: Brinell hardness (HBW 180–220 baseline) drops 5–10% to 170–200 HBW.

Cold-rolled SPA-H: Work-hardened hardness (HBW 210–270 baseline) drops 10–15% to 190–230 HBW.

Welded SPA-H: Hard, brittle HAZ hardness is normalized to the base metal's level, preventing hardness-induced cracking during secondary processing.

info-433-347

5. Property Uniformity & Dimensional Stability: Drastic Improvement

 

Homogenization: Eliminates cross-sectional property variations (e.g., harder HAZ in welds, softer core in thick hot-rolled plates) - strength, ductility, and toughness are consistent throughout the steel matrix, critical for large structural components requiring predictable performance.

Stress relief: Relieves 80–90% of residual stresses from rolling, cold forming, or welding, preventing long-term warping, dimensional distortion, or microcracking in precision applications (architectural cladding, sign panels, machined parts).