1. Pre-Folding Preparation: Protect the Base Surface and Oxide Layer

Retain the original protective film

 

Do not remove the factory-applied PE protective film on the weathering steel surface before folding. This prevents scratches or abrasions from the bending mold that would expose the unoxidized base metal (a major cause of localized rust).Choose mold materials carefully

 

Use polyurethane (PU) or nylon molds instead of hard steel molds. Hard steel molds can scratch the weathering steel surface; soft molds reduce friction and avoid damaging the initial rust patina or base material.Clean the surface in advance

 

Wipe the area to be folded with a dry, lint-free cloth to remove oil stains, dust, or debris. Oil residues will block uniform oxidation, while dust can cause uneven rusting after folding.

info-544-355

2. Folding Process: Control Parameters to Avoid Structural Damage

Strictly follow the minimum bend radius

 

As mentioned earlier, the bend radius directly affects the material's structural integrity. A radius that is too small will cause micro-cracks in the folded edge, allowing water, salt spray, and other corrosive media to penetrate.

For plates ≤3mm: Bend radius = 1–2× plate thickness

For plates 4–6mm: Bend radius = 2–3× plate thickness

For plates ≥8mm: Preheat to 200–300℃ first, then bend with a radius ≥3–5× plate thickness

Avoid over-bending and repeated bending

 

Repeated bending operations will cause fatigue damage to the steel, increasing the risk of cracks. Ensure the bending angle is accurate in one pass (e.g., 90° for flower box edges) to minimize stress accumulation.Deburr immediately after folding

 

Use a grinder, sandpaper, or deburring tool to remove sharp burrs, flash, or micro-cracks on the folded edge and corner. These burrs are prone to trapping moisture and causing pitting corrosion.

info-574-531

3. Post-Folding Treatment: Repair Oxide Layer and Block Corrosive Media

Repair damaged rust patina in time

 

If the surface oxide layer is scratched or worn during folding:

Clean the damaged area with a wire brush to remove loose debris.

Apply a weathering steel rust accelerator evenly on the area (choose a product matching the original rust tone).

Place the component in a controlled environment (60%–70% humidity, 20–25℃) for 2–3 days to form a uniform protective rust layer, ensuring consistency with the surrounding surface.

Seal crevices for outdoor/coastal applications

 

For folded edges used in high-humidity or coastal environments, apply a breathable anti-rust sealant to the fold crevice (do not cover the entire surface to preserve the natural rust aesthetic). This sealant prevents salt spray and water from accumulating in the crevice and causing intergranular corrosion.

Recommended sealant type: Silicone-based breathable sealant (compatible with weathering steel and non-toxic)

Avoid unnecessary painting or coating

 

Traditional paint will block the formation of the natural protective rust layer of weathering steel. Only use specialized weathering steel clear coats if long-term color stability is required (the clear coat is breathable and does not affect corrosion resistance).

info-742-532

4. Long-Term Maintenance: Reduce Corrosion Triggers

Avoid contact with incompatible materials

 

Do not directly contact the folded weathering steel components with materials such as ordinary carbon steel, copper, or aluminum. Galvanic corrosion will occur if they are in contact in a humid environment. Use insulating gaskets (e.g., rubber, plastic) for isolation if assembly is required.Regular cleaning for outdoor use

 

For outdoor components, rinse the surface with clean water every 3–6 months to remove accumulated dust, leaves, or other debris that can trap moisture. Do not use acidic or alkaline cleaning agents, which will damage the protective rust layer.

info-490-386