What is ASTM A847/A847M Standard?
ASTM A847/A847M is an American material specification covering cold-formed welded and seamless high-strength, low-alloy structural tubing with improved atmospheric corrosion resistance.
It applies to round, square, rectangular and special-shaped hollow sections used in welded, riveted or bolted construction of bridges, buildings and general structural applications.
The standard specifies chemical composition, tensile strength, yield strength, elongation, dimensional tolerances and testing requirements. ASTM A847 structural tubing has a minimum yield strength of 345 MPa and a minimum tensile strength of 485 MPa.
When exposed to suitable wet-dry atmospheric conditions, the steel develops a protective oxide layer that can reduce the need for conventional painting.
What is ASTM A847 Structural Steel Square Tube?
ASTM A847 structural steel square tube is a cold-formed high-strength, low-alloy weathering steel hollow section manufactured in square and rectangular configurations. It is designed for structural applications requiring a minimum yield strength of 345 MPa and improved resistance to atmospheric corrosion.
ASTM A847 square steel pipe can be manufactured through welded or seamless production routes, depending on the required dimensions and manufacturing capabilities.
Welded products are formed from flat-rolled steel and joined along a longitudinal seam, while seamless products are manufactured without a longitudinal weld seam. During cold forming, the steel strip is shaped into a hollow square or rectangular profile with controlled outside dimensions, wall thickness and corner radius.


Compared with conventional carbon steel hollow sections, ASTM A847 Corten square tube offers improved atmospheric corrosion resistance.
Its alloy composition supports the formation of a stable rust patina under suitable exposure conditions. This makes ASTM A847 cold formed square tube suitable for pedestrian bridges, highway bridges, outdoor structures, architectural frameworks, guardrails and exposed steel building components.
ASTM A847 Structural Steel Square Tube
Our ASTM A847 structural steel square tube is supplied for structural fabrication projects requiring controlled dimensions, high tensile strength and atmospheric corrosion resistance.
Available product configurations include square hollow sections (SHS) and rectangular hollow sections (RHS). We can discuss welded or seamless manufacturing routes, outside dimensions, wall thickness, cut lengths, end preparation and inspection requirements according to project drawings.
For exposed structural applications, appropriate drainage and detailing are required to prevent water accumulation inside hollow sections. Welding consumables and welding procedures should also be selected according to the base metal chemistry and the intended service conditions.
Get ASTM A847 Square Tube Stock List & Quotation
ASTM A847 Structural Steel Square Tube Specifications & Standards
|
Parameter |
Technical Specification |
|---|---|
|
Material Standard |
ASTM A847/A847M |
|
Material Type |
High-Strength Low-Alloy Weathering Steel |
|
Grade Designation |
ASTM A847 (No Grade Classification |
|
Product Type |
Structural Hollow Section (SHS/RHS) |
|
Cross-Section |
Square, Rectangular, Round, Special Shapes |
|
Manufacturing Process |
Cold-Formed Welded |
|
Welding Method |
ERW or EFW for applicable welded products |
|
Maximum Welded Periphery |
2,235 mm |
|
Maximum Welded Wall Thicknes |
25.4 mm |
|
Maximum Seamless Periphery |
813 mm |
|
Maximum Seamless Wall Thickness |
12.7 mm |
|
Minimum Yield Strength |
345 MPa (50 ksi) |
|
Minimum Tensile Strength |
485 MPa (70 ksi) |
|
Minimum Elongation |
19% (subject to specimen and wall thickness requirements) |
Chemical Composition of ASTM A847 Structural Steel Tube (wt.%)
ASTM A847 specifies chemical limits for carbon, manganese, phosphorus, sulfur and copper. Nickel, silicon and chromium are reported in the heat analysis because they are used in evaluating atmospheric corrosion resistance. They do not have individual minimum contents in the chemistry table.
|
Element |
Heat Analysis |
Product Analysis / 成品分析 (%) |
|---|---|---|
|
Carbon (C) |
≤ 0.20 |
≤ 0.24 |
|
Manganese (Mn) |
≤ 1.35 |
≤ 1.40 |
|
Phosphorus (P) |
≤ 0.04 |
≤ 0.04 |
|
Sulfur (S) |
≤ 0.035 |
≤ 0.045 |
|
Copper (Cu) |
≥ 0.20 |
≥ 0.18 |
|
Nickel (Ni) |
Report |
- |
|
Silicon (Si) |
Report |
- |
|
Chromium (Cr) |
Report |
- |
Mechanical Properties of ASTM A847 Corten Steel Square Tube
ASTM A847 structural square steel pipe is specified with minimum tensile properties for both round and shaped tubing. These mechanical requirements apply to square and rectangular hollow sections as well as round tubing.
|
Mechanical Property |
ASTM A847 Requirement |
|---|---|
|
Yield Strength |
≥ 345 MPa (50,000 psi) |
|
Tensile Strength |
≥ 485 MPa (70,000 psi) |
|
Elongation |
≥ 19% |
|
Test Gauge Length |
50 mm (2 in) |
|
Minimum Wall Thickness for 19% Elongation Requirement |
≥ 3.0 mm (0.120 in) |
Dimensional Tolerances of ASTM A847 Square and Rectangular Steel Tube
Dimensional accuracy directly affects the fabrication, welding, assembly and installation of structural hollow sections. ASTM A847 specifies dimensional tolerances for outside dimensions, wall thickness, length, straightness, squareness, corner radius and twist.
|
Item |
ASTM A847 Requirement |
|---|---|
|
Largest Outside Dimension ≤ 63.5 mm |
±0.5 mm |
|
Largest Outside Dimension 63.5–88.9 mm |
±0.6 mm |
|
Largest Outside Dimension 88.9–139.7 mm |
±0.7 mm |
|
Largest Outside Dimension >139.7 mm |
±1% |
|
Wall Thickness |
Minimum not more than 10% below specified; maximum not more than 10% above specified |
|
Squareness of Sides |
±2° maximum |
|
Outside Corner Radius |
≤ 3 × specified wall thickness |
|
Straightness |
10.4 × total length (m) ÷ 5 mm maximum |
|
Length ≤ 6.7 m |
+12.7 mm / −6.4 mm |
|
Length > 6.7 m |
+19.0 mm / −6.4 mm |
Manufacturing Process of ASTM A847 Cold Formed Square Tube
ASTM A847 cold formed square tube is manufactured through a controlled forming and tube-production process. The manufacturing route depends on whether the product is welded or seamless.
1. Raw Material Selection
Flat-rolled high-strength low-alloy weathering steel is selected according to ASTM A847 chemical composition and mechanical property requirements. Heat analysis reports are reviewed to verify carbon, manganese, phosphorus, sulfur, copper and other reported alloying elements.
2. Slitting and Preparation
For welded square steel pipe production, steel coils or plates are slit into strips according to the required tube perimeter and wall thickness. The strip edges are prepared for longitudinal welding.
3. Cold Forming
The prepared steel strip passes through a series of forming rolls to gradually produce a round or directly formed hollow profile. Subsequent sizing and forming operations establish the required square or rectangular cross-section.
4. Welding and Sizing
For welded ASTM A847 structural tubing, the longitudinal seam is joined using a suitable welding process, such as electric resistance welding or electric fusion welding. The tube then passes through sizing rolls to achieve the specified outside dimensions and sectional geometry.
5. Cutting and End Preparation
The formed tube is cut to the ordered length. Plain ends, beveled ends and burr removal can be arranged according to fabrication drawings and purchase requirements.
6. Inspection and Certification
Finished ASTM A847 square steel pipe is inspected for dimensional accuracy, mechanical properties, chemical composition and applicable manufacturing requirements. Material test certificates are provided according to the agreed certification requirements.



Atmospheric Corrosion Resistance of ASTM A847 Corten Square Tube
ASTM A847 Corten square tube is designed for structural applications exposed to atmospheric conditions. Its corrosion resistance is associated with the alloying elements in the steel and the formation of a protective oxide layer during alternating wet and dry exposure.
When exposed to suitable atmospheric conditions, the surface gradually develops a rust-colored patina. This layer can reduce the corrosion rate of the underlying steel compared with ordinary carbon steel. The development and stability of the patina depend on humidity, rainfall, drying cycles, air pollution, chloride concentration and structural detailing.
For ASTM A847 hollow square steel pipe, particular attention should be given to the following conditions:
Applications of ASTM A847 Structural Steel Square Tube
ASTM A847 structural steel square tube is used in structural projects where high load-bearing capacity and atmospheric corrosion resistance are required.
Its square and rectangular hollow profiles provide defined cross-sectional geometry for fabrication, bolted connections and welded structural assemblies.
Paleisbrug Den Bosch
1. Pedestrian and Highway Bridges
ASTM A847 square steel pipe can be used for bridge railings, structural supports, cross members and secondary framing exposed to atmospheric conditions.
2. Outdoor Pavilions
Corten square tube is used in columns, roof supports and exposed structural frames for outdoor shelters and pavilions.
3. Architectural Structures
Weathering steel square hollow sections are used in exposed columns, trusses, architectural frameworks and building support structures.
4. Guardrails and Guide Rails
ASTM A847 structural tubing can be incorporated into guardrail posts, guide rail supports and other exposed roadside structural components.
5. Sign and Lighting Supports
Square and rectangular steel hollow sections are used in sign posts, lighting supports and outdoor equipment frameworks.
6. Outdoor Fencing
Corten steel square tubes are used as fence posts, structural frames and supporting members in outdoor fencing systems.
Weldability of ASTM A847 Corten Steel Square Tube
ASTM A847 structural steel square tube is intended for welded, riveted and bolted structural construction. Welding procedures must be selected according to the steel chemistry, material thickness, joint configuration and intended service conditions.
For exposed weathering steel structures, matching weathering-steel welding consumables should be considered when the weld metal is also expected to develop a compatible patina. The welding procedure should address preheating requirements, heat input, interpass temperature and joint preparation according to the qualified Welding Procedure Specification (WPS).
|
Welding Consideration |
|---|
|
Base Material |
|
Welding Process |
|
Filler Metal |
|
Joint Preparation |
|
Preheating |
|
Interpass Temperature |
|
Weld Inspection |
Quality Control and Inspection of ASTM A847 Square Steel Pipe
Quality control of ASTM A847 structural steel square tube includes chemical composition verification, tensile testing, dimensional inspection, manufacturing inspection and applicable supplementary testing.
|
Test / Inspection Item |
Acceptance Criteria |
|---|---|
|
Chemical Analysis |
Meets applicable A847 chemical limits |
|
Tensile Test |
Yield ≥ 345 MPa; Tensile ≥ 485 MPa |
|
Elongation Test |
≥ 19% under applicable specimen conditions |
|
Dimensional Inspection |
Meets specified OD, wall, length and sectional tolerances |
|
Visual Inspection |
No unacceptable surface defects |
|
Flattening Test |
Applicable to round tubing |
|
Flaring or Wedge Crush Test |
Applicable when specified and within the relevant product scope |
|
Corrosion Resistance Evaluation |
Corrosion index ≥ 6.0 under referenced requirements |
|
Material Certification |
MTC with heat number and test results |
Lead Time, Packaging and Delivery
ASTM A847 structural steel square tube can be supplied according to project-specific dimensions, wall thicknesses, lengths and packaging requirements.
Production Lead Time: Confirmed according to order quantity, manufacturing route and size availability.
Cutting Service: Fixed-length cutting according to customer drawings.
End Protection: Protective caps can be provided when required.
Surface Protection: Bare mill finish or agreed protective treatment.
Packaging: Steel strapping and suitable wooden supports for transportation.
Marking: Material grade designation, standard, dimensions, heat number and batch identification according to the agreed marking requirements.
Documentation: Mill Test Certificate (MTC), packing list and other agreed inspection documents.
ASTM A500 Light Oiled Black Square Hollow Section Steel Tube Structural Steel Window Profiles S235jr Shs 2X2 Inch Thin Wall Steel Square Hollow Section Tubing - Square Steel Profile and Hollow Section Structural Steel
Contact Gnee For ASTM A847 Structural Steel Square Tube
Gnee supplies weathering steel products for structural fabrication, bridge construction and outdoor engineering projects. If you are sourcing ASTM A847 structural steel square tube, ASTM A847 square steel pipe or Corten square tube, our team can assist with material specifications, manufacturing routes, dimensional requirements and export arrangements.